| 斷裂伸長率 | 680% | 拉伸強(qiáng)度 | 15MPa | 密度 | 0.922g/cm3 |
| 熔體流動速率 | 4g/10min | 維卡軟化點(diǎn) | 90℃ | 規(guī)格級別 | 擠出 |
| 加工級別 | 擠出級 |
|
|
產(chǎn)品簡述
| 斷裂伸長率 | 680% | 拉伸強(qiáng)度 | 15MPa | 密度 | 0.922g/cm3 |
| 熔體流動速率 | 4g/10min | 維卡軟化點(diǎn) | 90℃ | 規(guī)格級別 | 擠出 |
| 加工級別 | 擠出級 |
詳細(xì)數(shù)據(jù)
訂購指南
| 性能項(xiàng)目 | 試驗(yàn)條件[狀態(tài)] | 測試方法 | 測試數(shù)據(jù) | 數(shù)據(jù)單位 | ||||
| 基本性能 | 熔體流動速率 | 190℃/2.16kg | ASTM D-1238 | 4 | g/10min | |||
| 密度 | ASTM D-1505 | 0.922 | g/cm3 | |||||
| 機(jī)械性能 | 拉伸屈服強(qiáng)度 | TD | ASTM D-882 | 109.2 | kg/cm2 | |||
| 拉伸斷裂強(qiáng)度 | ASTM D-882 |
|
kg/cm2 | |||||
| 拉伸模量 | 2%正割 | ASTM D-882 |
|
kg/cm2 | ||||
| 斷裂伸長率 | ASTM D-882 |
|
% | |||||
| 埃爾曼多夫撕裂強(qiáng)度 | ASTM D-1922 |
|
g | |||||
| 落鏢沖擊強(qiáng)度 | ASTM D-1709 | 123 | g | |||||
| 熱性能 | 熔點(diǎn) | ASTM D-2117 | 112 | ℃ | ||||
| 維卡軟化點(diǎn) | ASTM D-1525 | 90 | ℃ | |||||
| 脆化溫度 | ASTM D-746 | <-70 | ℃ | |||||
| 光學(xué)性能 | 霧度 | ASTM D-1003 | 14.6 | % | ||||
| 光澤度 | ASTM D-2457 | 34.6 | % | |||||